Dur aloi isel Llawlyfr electrod E8018-C2 Data sodro
CYDRADDOLDEB CEMEGOL:
ALLOY(wt%) | C | Mn | Si | Ni | Cr | Mo | P | S |
RHEOLAU GB/T | 0.12 | 1.25 | 0.80 | 3.00-3.75 | - | - | 0.03 | 0.03 |
RHEOLAU AWS | 0.12 | 1.25 | 0.80 | 3.00-3.75 | - | - | 0.03 | 0.03 |
GWERTH ENGHREIFFTIOL | 0. 045 | 0.75 | 0.22 | 3.52 | 0.04 | 0.06 | 0.007 | 0.004 |
EIDDO MECANYDDOL:
EIDDO | CRYFDER YIELD(MPa) | CRYFDER ESTYNIAD(MPa) | GWERTH IMAPACT J/℃ | ELONGATION(%) | Triniaeth wres ° Cxh | |||||
RHEOLAU GB/T | 460 | 550 | 27/-75 | 17 | 605*1 | |||||
RHEOLAU AWS | 460 | 550 | 27/-75 | 19 | 605*1 | |||||
GWERTH ENGHREIFFTIOL | 495 | 600 | 100/-75 | 26 | 605*1 |
PARAMEDRAU WELDIO A ARGYMHELLIR:
MANYLEBAU DIAMETER(mm) | 2.6*350 | 3.2*350 | 4.0*400 | 5.0*400 | ||||
TRYDAN (Amp) | H/W | 80-110 | 100-130 | 130-180 | 170-210 | |||
O/W | 60-100 | 80-120 | 120-160 | - |
Haearn powdr electrod llaw math hydrogen isel.
Oherwydd ychwanegu powdr haearn, mae'r effeithlonrwydd toddi yn uwch, mae caledwch effaith y metel tawdd ar -75 ℃.
Arc sefydlog, llai o sblash, ffurfio da, tynnu slag yn hawdd, mae perfformiad X-Ray yn ardderchog.
CYDRADDOLDEB CEMEGOL:
ALLOY(wt%) | C | Mn | Si | Ni | Cr | Mo | P | S |
RHEOLAU GB/T | 0.12 | 1.25 | 0.80 | 3.00-3.75 | - | - | 0.03 | 0.03 |
RHEOLAU AWS | 0.12 | 1.25 | 0.80 | 3.00-3.75 | - | - | 0.03 | 0.03 |
GWERTH ENGHREIFFTIOL | 0. 045 | 0.75 | 0.22 | 3.52 | 0.04 | 0.06 | 0.007 | 0.004 |
EIDDO MECANYDDOL:
EIDDO | CRYFDER YIELD(MPa) | CRYFDER ESTYNIAD(MPa) | GWERTH IMAPACT J/℃ | ELONGATION(%) | Triniaeth wres ° Cxh | |||||
RHEOLAU GB/T | 460 | 550 | 27/-75 | 17 | 605*1 | |||||
RHEOLAU AWS | 460 | 550 | 27/-75 | 19 | 605*1 | |||||
GWERTH ENGHREIFFTIOL | 495 | 600 | 100/-75 | 26 | 605*1 |
PARAMEDRAU WELDIO A ARGYMHELLIR:
MANYLEBAU DIAMETER(mm) | 2.6*350 | 3.2*350 | 4.0*400 | 5.0*400 | ||||
TRYDAN (Amp) | H/W | 80-110 | 100-130 | 130-180 | 170-210 | |||
O/W | 60-100 | 80-120 | 120-160 | - |
Ysgrifennwch eich neges yma a'i hanfon atom